Our Services
Concrete Thermal Modelling and Cracking Control
Cement hydration in concrete is an exothermic
reaction and as a result concrete temperature can rise significantly in the
early age maturing if the heat is not dissipated into the environment. Such
rise in temperatures has many adverse consequences especially for the thick
elements, with steam curing or high level of insulation. .
If the temperature is higher than a certain
limit (e.g. 70 °C for GP cement and 80 °C for blend cements) the a unstable
cement hydration product (monosulphoaluminate phase called AFm) can form and it
will transfer into ettringite (AFt) phase with significant volume
increase. Such an expansion process will
disintegrate the concrete matrix causing premature distress.
In addition, the strength of concrete in early
age experiencing high temperature will form coarse crystal grains with significantly lower strength compared to those
cured in normal temperatures. It is
critical to control concrete peak temperature below the limits so that the
durability is not compromised. The best
practice is to conduct thermal modelling using CIRIA C660 or C766 to predict
temperature rise considering the specific structure dimension, configurations,
reinforcement details, concrete mix characteristic, formwork type, retention
time and ambient conditions.
In addition, the high early age temperature in
concrete under external restraint can also expand while concrete has a good
plasticity. After peak temperature, the
temperature of concrete decreases gradually when contraction occurs. However,
the contraction of such a hardened concrete may be restrained by the joining
elements (such footing or base slab) constructed early. Tensile strength will develop and if the
stress is greater than the concrete tensile strength, which is very low at
early age, cracking will occur through the entire depth of the elements.
Such cracks are permanent and may grow in width
with increasing drying shrinkage. It is
important to control such cracks as the durability will be compromised with
such cracks especially in aggressive conditions. The thermal modelling can be used to estimate
external restraint and assess the cracking risk so that preventive measures can
be selected and adopted.
Another consequence of high peak temperature in
concrete with insufficient insulation/formwork is a high temperature
differential between surface and centre of concrete elements. Concrete has a relatively low thermal
conductivity and heat transfer is slow within elements. Cooling is fast on surfaces with a lower
temperature than the centre and the contraction of surface concrete is
restrained by the centre hot concrete, tensile stress thus develops. The stress level increase with temperature
differential and at a certain differential, stress exceeds tensile strength and
cracking occurs. The maximum allowable
differential to avoid cracking decreases with coefficient thermal expansion of
concrete related to aggregate type.
To avoid cracking risk under internal restraint,
BAE’s engineers have the leading expertise in such thermal modelling work and
have successfully delivered numerous thermal
reports in Australia and abroad. In addition, more advanced models than the
original CIRIA C660 model have been developed by BAE’s engineers to predict
temperatures in concrete with cooling pipe systems and in cylinder elements
with radial heat transfer to ground.
Furthermore, the model to estimate the edge
restraint of pile-caps or headstock by spaced piles or pier columns are also
developed and used in many projects. We
have also developed unique solutions to reduce the external restraint level by
construction sequential. We have also adopted a sophisticated method to
estimate heat of cement hydration curve by analysing the results from hot box
testing of concrete blocks.
The early age thermal modelling techniques can
be also used to determine the causes of cracking in various concrete
elements. BAE’s engineers have rich
experience in cracking investigations on causes of cracking in some concrete
elements such as concrete water tanks, pavement slabs, bridge decks, toppings
and warehouse slabs.
We monitored the temperature history in various
concrete and metal elements such as large thick raft slab, large pile-caps, hot
box concrete blocks, and building slabs etc. We have used datalogging system in
most the cases to obtain accurate and continuous data in-situ or remotely. The results can be used to determine the
current performances of the elements and whether there is any abnormal behaviour.
The results of hot box testing can be used to
determine the adiabatic temperature rise curve in concrete. It is the critical information for concrete
early age thermal modelling and cracking analysis and control/prevention.